Skip to content
5axes edited this page Nov 11, 2021 · 7 revisions

With the right flow rate, your top and bottom layers should look great. The small circle must be also visible.

This test will creates 11 parts with a specific Flow rates already associated with the part.

SCAD Multi Flow Test Model

Multi Flow Test

Printing Conditions

 - Nozzle Size : 0.4
 - Layer Height : 0.2
 - Initial Layer Height : 0.2
 - Line Width : 0.4
 - Wall Line Count : 2
 - Top/Bottom Thickness : 0.8 mm

Printing Time = 45mn

Instructions

Print the tests parts if you don't want to print every part you can remove the part with the flow rates you don't want. After the print is finished, check the quality of your top and bottom layers. Use the flow rate of best part for your print.

Use the automatic reorder function to arrange every parts on the build plate (CTRL+R).

Print the test part and choose the flow with the best result : Multi Flow Test Result

On this test a flow at 90% looks like the best result : Multi Flow Test detail

Clone this wiki locally